Time-dependent anelastic deformation mechanisms arise in austenitic stainless steel when load is removed during a high-temperature creep test. This phenomenon is investigated by conducting creep tests, with intermittent load removal, on AISI Type 316H austenitic stainless steel at 550 and 650°C, supported by in situ measurement of creep-induced intergranular residual strains by neutron diffraction. All the cyclic tests exhibit anelastic behaviour on unloading and develop substantially lower load-on creep strain rates, reduced ductility and longer rupture times than baseline steady-load creep tests at similar conditions. The mechanisms underlying the observed anelastic behaviour and changes in macroscopic creep properties are discussed with reference to the development of intergranular strains and dislocation behaviour.