Positive temperature coefficient of resistivity (PTCR) effect and electrical properties of (Ban-xSmx)TiO3(BSMT ) samples with different Ba-site/Ti-site ratio (n) and various concentration of the donor-doped Sm3+(x) sintered in a reducing atmosphere and reoxidized in air are investigated. The results show that the room temperature resistivity (ρRT) of the semiconducting BSMT ceramics first decreases and then increases with increasing of concentration of the donor-doped Sm3+, especially whenxis 0.005 mol, the ρRTof the BSMT ceramics is the lowest. Moreover, the ρRTof the Ba-excess BSMT (n= 1.01) specimens reoxidized at 800 oC for 1 h after sintering at 1270 °C for 30 min in a reducing atmosphere is lower than the Ti-excess ones (n= 0.99), in addition, the ρRTof the BSMT specimens increases with an increase of both sintering temperature and reoxidized time.