The property of Heavy axial forgings can be modified by the reasonable drawing process with the advantage of dynamic recrystallization. In view of formation, heat transfer, heating generation, dynamic recrystallization a macro-micro coupled process was modeled, and the drawing process of φ300 mm×4000 mm axial forging is simulated .It is found that when the cumulative reduction ratio reaches 9% in the second round, the dynamic recrystallization occurred in the material as it reached a critical strain condition .With the reduction ratio increases, the volume fraction of dynamic recrystallization increases. When the cumulative reduction ratio reaches 60%, about 67% of the inner region of the axial forging is modified fully. After the drawing process, the dynamic recrystallization grain size in 60% of the cross-section area is less than 100 μm , and the grains get refined.