Abstract

This short communication determines the strength of two glass polyalkenoate cements that differ from each other through the composition of their glass phase. Sample sets of n=5, 10, 20 and 30 were formulated and tested in biaxial flexure. The derived mean for each sample set was compared against the Weibull characteristic strength. The mean and corresponding characteristic strength show a maximum percentage difference 10.1%, and the 95% confidence intervals calculated from the mean data encompass the corresponding characteristic strength down to a sample set of n=5. This suggests that, for brittle materials such as glass polyalkenoate cements, it is acceptable to test only five samples of each material in biaxial flexure and the resultant 95% confidence intervals will encompass the corresponding Weibull characteristic strength of the material.