Abstract

The paper focuses on the use of glass waste as a substitute for aggregates (0/4, 4/8 and 8/16 mm) in the production of concrete in order to reduce the negative impact of existing waste on the environment. For the study, 5 mixtures were designed with gradual replacement of individual natural aggregate fractions in the concrete mixture by glass cullet. Real density, total water absorption and compressive strength were monitored on cubes with an edge of 100 mm for a period of 14 days to 3 years. The achieved compressive strength of samples with glass as a filler at the level of 50 MPa gives a good precondition for the real use of such concrete in practice. In addition, when combined it with lower real density and total water absorption.