The steam oxidation behavior of solid solution strengthened alloy 617 at 900 °C-1100 °C was investigated. The oxidation products were characterized by scanning electron microscopy, X-ray diffraction, and energy-dispersive spectroscopy. The results show that the oxidation kinetics of alloy 617 in steam followed the parabolic oxidation law. The calculated activity energy of alloy 617 was 223.47 kJ/mol. The oxidation products were mainly composed of external and internal scales and prior oxides at grain boundaries. External oxide scales were MnCr2O4, TiO2, and Cr2O3. Internal oxidation scales and prior oxides were Al2O3 and some Cr2O3 dissolved into Al2O3. The growth mechanism of oxide scales on alloy 617 is proposed.