The present work investigate the possibility of obtainment by mechanical alloying of Ni superalloys based on the Ni-Cr-Nb-C system strengthened by γ”(Ni3Nb), since γ”(Ni3Nb) as γ’ (Ni3Al) are typical coherent phase strengthening mechanisms in nickel superalloys. In order to evaluate this possibility, a composition with 71,65wt%Ni, 7,90wt%Cr, 20,00wt%Nb and 0,45wt%C was processed in a SPEX mill by 8 hours, consolidated and sintered at different temperatures (1200oC, 1250oC and 1300oC). The powder processed by MA and the sintered products were characterized by x-ray diffraction, SEM and EDS.