Abstract

The leaching process of copper from calcareous bornite ore using ammonium persulfate as an oxidant in ammoniacal solution was investigated. The effects of stirring speed, temperature, initial concentration of ammonia and ammonium persulfate, and liquid-to-solid (L/S) ratio on the extraction percentage of copper from bornite ore were studied. The results show that the optimum leaching conditions for bornite ore with a maximum extraction of copper 88.9 pct are temperature 313.15 K (40 °C), reaction time 4 hours, stirring speed 600 r/min, L/S ratio 7/1 cm3/g, initial concentration of ammonia 2.0 mol/dm3, and ammonium persulfate 3.0 mol/dm3.