This paper presents the first results for irradiation of tungsten, molybdenum and stainless steel samples with the 4 kJ plasma focus (PF) device at the University of Sofia. The samples were placed 4 cm above the anode of the PF machine and were exposed to a considerable number of shots. The working gas was deuterium with the pressure adjusted in the range of 1–3.3 mbar. Thus, the plasma streams and the fast-ion beam, which appear after the pinch phase, impinge the samples. The interaction of the pinch products with the targets causes substantial surface damage to the specimens. A mesh of partially melted cracks and re-crystallized regions are revealed on this surface and various chemical compounds are also present.