Abstract

The chemical durability of lead glass tumblers (24% PbO) in a 4% (v/v) acetic acid solution before and after coating with sol-gel derived SiO2 films was assessed to determine the extent of reduction in Pb-leaching that can be achieved. It was found that by coating the internal surface of the glass tumblers with 1 ml of 10% TEOS solutions at 100°C and densifying the coating formed at 500°C for 1 h, it was possible to reduce Pb-leaching to about one quarter of that of the uncoated glass.