Abstract

The selective oxidation of Si, Mn, and B on TRIP steel surfaces is a widely known phenomenon that occurs during heat treatment. However, the relationship between oxide formation and the annealing factors is not completely understood. This study examines the effect of the annealing conditions (dew point and annealing temperature) on oxide formation. A low dew point of −40 °C leads to the formation of Si-based oxides on the surface. A high dew point of −20 °C changes the oxide type to Mn-based oxides because the formation of Si oxides on the surface is suppressed by internal oxidation. Mn-based oxides exhibit superior wettability due to aluminothermic reduction during galvanizing.