The article discusses the physical and mechanical regularities of ceramics formation based on the BaO—Al2O3—SiO2 system by slip casting into gypsum molds, and also investigates the rheological properties of a slip based on сelsian and the physicochemical properties of products made from it.
 The samples were made according to the following technology: the first stage is synthesis of celsian in a muffle furnace at a temperature of 1200 °C with a maximum temperature holding for 2 hours. The synthesis products were ground in a planetary mill to a residue on the № 0063 sieve of no more than 0.2 %. Then, slips with different moisture content without additives and with the addition of 0.10, 0.15 and 0.20 wt. % thinning additive Dolapix PC 67 were made. The second stage is to obtain samples by casting slip into gypsum molds. Firing of products took place in a muffle furnace at a temperature of 1350 °C with a two-hour holding.
 The optimal amount of thinning additive in the celsian slip was determined, which corresponds to 0.10 wt. %. It was found that, in the studied area of technological parameters, the material acquires the best properties at a sample firing temperature of 1350 °C and is characterized by the following indicators: water absorption — 10.20 %, apparent density — 2.15 g/cm3, open porosity — 21.04 %.

Full Text
Published version (Free)

Talk to us

Join us for a 30 min session where you can share your feedback and ask us any queries you have

Schedule a call