Abstract

In the present study lateritic nickel ore was used for bacterial leaching using a mixed consortium of mesophilic acidophiles. The microorganisms were adapted to 1 gram nickel/L prior to leaching. For the experiments, lateritic ore in different forms such as raw, roasted, roasted ore presoaked in dilute sulphuric acid and palletized pretreated roasted (400 °C and 600 °C) ore were taken. The leaching experiments were conducted in 9 K+ with 40 L capacity bioreactor using 10% (v/v) inoculum concentration at 10% (w/v) pulp density. The aeration was maintained at 2–3 L/min and the speed of agitator and temperature at 400–500 rpm and 35 °C. The maximum extraction of nickel and cobalt was observed with pretreated ore (600 °C) at 10% pulp density (77.23% and 73.22%) respectively within 31 days at pH 1.5 and least extraction in case of raw ore i.e., 9.47% nickel and 41.12% cobalt respectively.