Magnets from Sm3(Fe0.93Ti0.07)29 material were prepared from powder, which was milled, carburized or nitrided, then field compacted in a die press and resin-bonded. Both types of magnet exhibit coercivities of about 0.4 T. The coercivity can be increased up to 0.9 T by additional milling after nitrogenation. Zn-bonding of these powders seems to be less effective for enhancing the coercivity than for Sm2Fe17 interstitials.

Full Text
Paper version not known

Talk to us

Join us for a 30 min session where you can share your feedback and ask us any queries you have

Schedule a call

Disclaimer: All third-party content on this website/platform is and will remain the property of their respective owners and is provided on "as is" basis without any warranties, express or implied. Use of third-party content does not indicate any affiliation, sponsorship with or endorsement by them. Any references to third-party content is to identify the corresponding services and shall be considered fair use under The CopyrightLaw.