Abstract
In this paper, tests and analysis of thermal runaway propagation for commercial modules consisting of four 41 Ah Li-ion pouch cells are presented. Module samples were tested at 100% state-of-charge and mechanically constrained between two steel plates to provide thermal and mechanical contact between the parts. Voltage and temperature of each cell were monitored during the whole experiment. The triggering of the exothermal reactions was obtained by overheating one cell of the stack with a flat steel heater. In preliminary studies, the melting temperature of the separator was measured (from an extracted sample) with differential scanning calorimetry and thermogravimetric analysis techniques, revealing a tri-layers separator with two melting points (≈135 °C and ≈170 °C). The tests on module level revealed 8 distinct phases observed and analyzed in the respective temperature ranges, including smoking, venting, sparkling, and massive, short circuit condition. The triggering temperature of the cells resulted to be close to the melting temperature of the separator obtained in preliminary tests, confirming that the violent exothermal reactions of thermal runaway are caused by the internal separator failure. Postmortem inspections of the modules revealed the internal electrical failure path in one cell and the propagation of the internal short circuit in its active material volume, suggesting that the expansion of the electrolyte plays a role in the short circuit propagation at the single cell level. The complete thermal runaway propagation process was repeated on 5 modules and ended on average 60 s after the first thermal runaway triggered cell reached a top temperature of 1100 °C.
Highlights
Propagation speed of thermal runaway (TR) in a Li-ion battery module is an important phenomenon to consider as part of the battery pack design process
The process occurring at lower temperatures around 100 ◦ C likely corresponds to the shrinking of the polyolefin part of the separator; water evaporation may contribute in this temperature region
Li-ion cells were triggered to TR—by overheating the first cell of the stack—and the evolution observed by voltage and temperature sensors
Summary
Propagation speed of thermal runaway (TR) in a Li-ion battery module is an important phenomenon to consider as part of the battery pack design process. The exothermal behavior of the TR can change if the cell is triggered under different abuse conditions [9,10,11,12,13]; as a consequence, the initiation of TR is a fundamental aspect to consider to obtain test results in the direction of the desired target. If the initiation is induced externally, for example, by a mechanical actuator (i.e., nail penetration), its exothermal behavior could be very different with respect to the triggered cells (induced by cascade effect), likely causing a difference in propagation velocity. The triggering method must be robust and exhibit good repeatability
Talk to us
Join us for a 30 min session where you can share your feedback and ask us any queries you have
Disclaimer: All third-party content on this website/platform is and will remain the property of their respective owners and is provided on "as is" basis without any warranties, express or implied. Use of third-party content does not indicate any affiliation, sponsorship with or endorsement by them. Any references to third-party content is to identify the corresponding services and shall be considered fair use under The CopyrightLaw.